Technological Parameters Choice of Rail Flash Butt Welding
發(fā)布時(shí)間:2024-10-09瀏覽次數(shù):430


Reasonable technological parameters are the guarantee of high quality flash butt welding joint. Reasonable technological parameters can not only ensure the high quality welding joint of low carbon steel workpiece, but also can make some metal workpiece with poor weldability get satisfactory quality of joint.

Welding Voltage and Current      

Reasonable welding current is the necessary condition of stimulating flash and maintain stable process of flash, usually we use current density (the current which through unit binding surface) represents the welding condition level. Usually, flash butt welding current density is 10-25ampere/millimeter. If current density is too small, rate of heating is low, flash butt can not be stimulated quickly or the process of flash butt is not steady. If current is too large, the process of flash butt welding will be too fierce, there will be deeper fire-pit on welding edge face, when upset, it is difficult to seal up them, and thereby there is defects. If current is too large, the process of flash butt welding will be too fierce, this can make the temperature field of welding   excessive, when upset, it is not easy to make plastic deformation and then reduce the quality of joint. When volume-produce mild steellow alloyed steel joint, usually choose upper limit value of current density.  After the butt-welding machine is defined, the current of the joint is determined by voltage.  Change the gear of closing primary coil tap of welding transformator, then change the welding voltage and current (sometimes stepless regulation of the welding voltage).

Burn-off rateFeed rate      

The burn-off rate of flash butt welding is determined by welding current densitypreheat degree and some other factors of workpiece chemical constituents. The heat produced on the interface between two workpieces when flash butt welding, the temperature of workpiece enhances with the increase of flash and the burn-off rate enhances with the increase of workpiece’ temperature . The feed rate must compatible with burn-off rate of the workpiece. If the feed rate is greater than burn-off rate, the two interfaces of the workpiece will short-circuited. Because the burn-off rate enhances with the increase of workpiece’ temperature, the feed-in of workpiece should be accelerated motion, and the motion curves should be nearly constant around the parabola. 

Combustion Allowance      

Combustion allowance is the lost length of workpiece in the process of flash-butt injection. Combustion lost must be considered when butt welding to ensure the length of the workpiece meets the design requirement. The basis which determines the combustion is: the allowance must be enough to ensure when the process of combustion finished, there should be even heating on all end faces of the two weldments, and the extent of heating should make plastic deformation in the process of upsetting to get high quality joints. The larger interfacial areas of the weldments, the slower homogenization rate of the temperature on the contact face, and the flash (combustion) time is longer, combustion allowance is larger. If pre-heating mean is carried out, the temperature of interface is higher, and there is temperature homogeneous diffusion to the whole interface, in the process of flashing, the time of temperature homogenization will be shortened, and then the combustion allowance will be smaller. To the steel parts of which section is round in shape, when the continuous flash welding is adopted, the combustion allowance (the sum of burned value of the two workpieces) normally is (0.6—0.7) d, when the preheating flash butt welding is adopted, the combustion allowance is (0.4—0.5) d, (D is the diameter of the workpiece).

Upset Allowance

Upset allowance is the shortening of the workpiece in the process of upsetting.

      (1) Molten metal and metallic oxide must be crowded to the surface of the workpiece

      (2) Metals of the two interfaces must close contact at the whole cross section. That is the contact parts of the two workpieces should produce sufficient plastic deformation. If the upset allowance is smaller, it is the main cause for the defects of shrinkage cavity inside the joint, cast structure, grey speck, oxide inclusion and incomplete penetration. If the upset allowance is larger, excessive plastic metal will be squeezed, and increases the difficulty in eliminating joint burr. In order to make sure the hot metal (liquid state) of the binding surface not is oxidized, and supplement the subcooling in the process of flash butt, the power should not be cut off before the upsetting, but in the process of upsetting. The upset process before the power is cue off is called charging upset; the subsequent process is called electroless upset. So in fact, the upset allowance is the sum of charging upset and electroless upset, and charging upset accounts for the whole upset allowance of 30%--40%.

Upset Speed

If there is flash butt welding, a normal tendency is for larger upset speed to crush out the molten metal before the solidification, and upset in the optimum breach when the metal has good plasticity. High upset speed will reduce the risk of oxidizing hot metal to get high quality welding joints. Usually, the upset speed is no less than 20mm / s.  Hydraulic rotary transmission welding machine generally has large upset speed, its upset speed can reach 60 mm / s.

Extension

Extension is the protruding length of workpiece from the clamp jaw (conductor). After fixturing, the distance between two conductors is the whole extension; its value is the sum of the extensions of two workpieces. When the section surface and material trademark are same, its extension is the half of the whole extension. When weld different materials workpieces, the speed of melting will be different in the process of flash butt because of different conductivity, thermal coefficient and melting point. If fixturing at the moment, the extension of the fast melting workpiece is larger than the extension of the other one.  When weld metal piece of which cross section is round in shape, the whole extension is normally (1—1.4) d, (D is the diameter of the workpiece).



主站蜘蛛池模板: 加勒比色老久久爱综合网 | 久久色婷婷 | 蜜桃视频在线观看www社区 | 国模丽丽啪啪一区二区 | 成人做爰视频WWW网站 | 嫩草影院地址 | 18禁美女黄网站色大片免费看 | 国产欧美色一区二区三区 | 中文字幕无码人妻少妇免费 | 女社长被下属捆绑调教 | 免费AV无码不卡在线观看 | 最近的2019免费中文字幕 | 2020精品国产自在现线看 | 人妻AV无码一区二区三区 | 少妇三级全黄 | 重囗另类BBWSeⅹHD | 亚洲欧美乱日韩乱国产 | 欧美在线激情 | 国产日产精品_国产精品毛片 | 亚洲精品久久久久AV无码 | 四虎影视免费 | 色偷偷AV男人的天堂京东热 | 香蕉成人国产精品免费看网站 | 在线看免费无码AV天堂 | 久久亚洲AV成人网站玖玖 | 无套内谢少妇毛片A片 | 韩国免费a级毛片久久 | 黑人啊灬啊灬啊灬快灬深 | 亚洲精品无码高潮喷水A片小说 | 正在播放国产一区二区 | 亚洲Av永久无码精品无码流畅 | 色噜噜狠狠爱综合视频 | 丁香五月开心婷婷综合中文 | 无码人妻精品一区二区三区欧美 | 波多野42部无码喷潮在线 | 成年女美黄网站大全免费播放 | 老师您的兔子好软水好多樱花国漫 | 福利视频欧美一区二区三区 | 日韩福利片午夜免费观着 | 久久人人爽人人爽人人片AV麻烦 | 经典老熟女ass |